KILN CONNECTION: Elegant Burner Concept

Table 1. Heat available when firing with a cubic foot of natural gas at varying rates of XSA and preheated air temperature.

One of my strong interests is energy conservation, and it is something that I focus on for almost all of my clients. The volatility of natural gas costs over the past 10 years should demonstrate that the only way to reduce exposure to costs that you cannot control is to try to minimize them.

Unfortunately, the thermodynamics of combustion ensure that you never get all of the fuel that you pay for. Generally, a cubic foot of natural gas contains about 1000 BTUs, but the heat available to do what you want it to -- which is to heat the kilns -- is much less, depending on a variety of factors.

If you use excess air (XSA), you pay a penalty to heat the air in excess of the combustion needs. And as the temperature of your process rises, the available heat also declines drastically. Table 1 indicates the drastic differences in available heat when firing with a cubic foot of natural gas at varying rates of XSA and preheated air temperature.

You can often reduce XSA, but you are stuck with your process temperature. So what can you do? The table shows that preheating the combustion air has a major impact, but this can be very costly, difficult and cumbersome, with oversized combustion air piping, insulation, recuperator installation in the exhaust flue, and ratio inaccuracies resulting from changing air properties. Because of a tunnel kiln's recuperative properties, higher-temperature zones exhaust into cooler zones; therefore, the chart overstates the effective savings. But in a periodic kiln, where the kiln exhausts at process temperature, the savings can be spectacular. In addition, if there is incineration on the periodic kiln, the reduction in exhaust gas flow due to preheated air results in savings there as well.

One option for preheated air is to use oxygen enrichment as a means of increasing the effective BTU value/efficiency, and this solution can also be effective. Unfortunately, oxygen is expensive. Several projects that I have worked on net similar savings when the combustion air is enriched to 25% O2, but about half of that savings ends up being lost by paying for the oxygen use.

Therefore, preheated air is a desirable solution, but one that quite often requires investment in the recuperator, piping, controls, etc. Another interesting option is available, however, and I admit that I need your help to explore it.

Self-Recuperating Burners

Some companies manufacture burners that "self recuperate" -- they withdraw a fraction of the kiln exhaust gases around the periphery of the burner nozzle. This hot exhaust air heats the incoming combustion air inside the burner with a mini-heat exchanger, generating preheated air without the complication of normal methods.

This concept is simply elegant, and though it needs a burner exhaust collection system, the piping can be relatively simple. I do have some questions, however, including:
  • What is the impact on the process temperature uniformity when exhaust gases are exhausted from many different sites?
  • What means are used to control ratio accuracy in this system, with widely variable combustion air temperatures?
  • What is the burner life (any impact on the burner maintenance, etc.)?
Do you have experience with this kind of system? If so, please contact me. I would love to hear your comments, both pro and con, since energy conservation is one of the best means of saving money, reducing CO2 and staying competitive. If I can use your comments, I will refer to your generosity when providing assistance to others in our field

Did you enjoy this article? Click here to subscribe to Ceramic Industry Magazine.

Ralph-ruark-107px

Ralph Ruark is president of Swindell Dressler International. He was formerly president of Ruark Engineering, Inc., a company that provided analysis, recommendations and training for clients worldwide that manufacture industrial ceramics. He can be reached at (412) 788-7100 or rruark@swindelldressler.com.

Recent Articles by Ralph Ruark

You must login or register in order to post a comment.

Multimedia

Videos

Podcasts

Thermal Processing Optimization: Using Advanced Rotary Tube Internals

Mike Maggio of Harper International discusses rotary tube internals with Susan Sutton, editor-in-chief.

More Podcasts

THE MAGAZINE

Ceramic Industry Magazine

CI May 2013 cover

2013 May

The 2013 May Ceramic Industry includes articles on treating heat like light, recycling, solar energy, and more. Check it out today!

Table Of Contents Subscribe

THE CERAMIC INDUSTRY STORE

M:\General Shared\__AEC Store Katie Z\AEC Store\Images\Ceramics Industry\handbook of advanced ceramics.gif
Handbook of Advanced Ceramics Machining

Ceramics, with their unique properties and diverse applications, hold the potential to revolutionize many industries, including automotive and semiconductors.

More Products

Clear Seas Research

Clear Seas ResearchWith access to over one million professionals and more than 60 industry-specific publications,Clear Seas Research offers relevant insights from those who know your industry best. Let us customize a market research solution that exceeds your marketing goals.

Directories

0711ci_cover.gif

Ceramic Industry's Directories including Components, Equipment Digest, Services, Data Book & Buyers Guide, Materials Handbook and much more!

STAY CONNECTED

facebook_40px twitter_40px  youtube_40pxlinkedin_40